Aluminum alloy die-casting is one of the most efficient metal-forming technologies. It has the advantages of high production efficiency, complex casting, and high precision. Therefore, it is widely used in the automotive industry, aerospace, 5G communication equipment, and other fields. With the development of modern industry, aluminum alloy die-casting processes and die-casting equipment have been continuously upgraded, and various industries have increasingly higher requirements for the quality, performance, and accuracy of die-cast aluminum component products.
Compared with other casting technologies, the surface of die casting is smoother and has higher dimensional consistency. However, in order to obtain a die casting with a perfect surface, you need to master the surface treatment process of the entire die casting process, otherwise, the die casting will be damaged. A series of surface defects are generated, which not only affect the appearance of the product but also affect the use effect of the product to a certain extent.
Appearance defects of die castings
Die casting is a metal casting process characterized by using a mold cavity to apply high pressure to molten metal, similar to injection molding of plastics. Die casting is particularly suitable for manufacturing large quantities of small and medium-sized castings, so die casting is the most widely used among various casting processes. Compared with other casting technologies, die casting has a flatter surface and greater dimensional consistency. However, irregular operations and parameters can also produce a wide variety of defects.
First-class marks and patterns
There are stripes on the surface of the casting that are consistent with the flow direction of the molten metal, and there are clearly visible non-directional lines that are different in color from the metal matrix and have no development trend.
The reasons for flow marks are as follows:
- The mold temperature is too low.
- Poor runner design and poor location of the inner gate
- The material temperature is too low.
- The filling speed is low and the filling time is short.
- The pouring system is unreasonable.
- Poor exhaust;
- The spray is unreasonable.
Two reticulated hairy wings (turtle cracks)
There are raised or depressed marks on the surface of the die-casting parts, like hairlines, which continue to expand and extend as the number of die-castings increases.
The reasons are as follows:
- There are cracks on the surface of the die-casting mold cavity;
- The die-casting mold is not evenly preheated.
Three cold partitions
The surface of the die-casting parts has obvious, irregular, sunken linear lines (both penetrating and non-penetrating), which are small and narrow in shape. Sometimes the intersection edges are smooth, and there is a possibility of disconnection under the action of external force.
The reasons are as follows:
- The two metal streams are connected to each other, but they are not completely fused, there is no inclusion between them, and the bonding force between the two metal streams is very weak.
- The pouring temperature or die-casting mold temperature is low.
- The sprue position is incorrect or the flow path is too long.
- The filling speed is low.
Four dents
A relatively thick aluminum casting with smooth indentations (like a dish) on most surfaces
The reasons are as follows:
- Improper design of die-casting parts due to shrinkage; too large wall thickness difference; inappropriate sprue position;
- The injection specific pressure is low and the holding time is short; the local temperature of the die-casting mold is too high.
- The cooling system design is unreasonable.
- Open the mold too early.
- The pouring temperature is too high.
five marks
Marks left by the contact between the surface of the casting and the surface of the die-casting model cavity or step marks on the surface of the casting.
The reasons are as follows:
- The end face of the ejector rod is worn due to the ejection component; the adjustment length of the ejector rod is inconsistent;
- The splicing part of the die-casting model cavity does not fit well with other parts.
- The inserting part is loosened due to splicing or movable parts; the movable part is loosened or worn; the side wall surface of the casting is formed by the inserts of the moving and fixed molds interpenetrating each other.
Six traces of adhesions
Small flakes and the base part of metal or non-metal are welded to the metal, and the small flakes peel off under the action of external force. Some of the surfaces of the peeled castings are shiny and some are dark gray.
The reasons are as follows:
- There are metal or non-metallic residues on the surface of the die-casting model cavity;
- During pouring, impurities are first brought in and attached to the surface of the cavity.
Seven layers (skin-fitting and peeling)
Appearance inspection or damage inspection: There are obvious layers of metal in parts of the casting.
The reasons are as follows:
- The mold is not rigid enough and the template will vibrate during the filling process of molten metal;
- The punch crawls during the injection process;
- Improper design of the sprue system.
8 Friction ablation
The die casting surface produces rough surfaces in certain locations.
The reasons are as follows:
- Improper position, direction and shape of the ingate caused by the die-casting mold (mold);
- Insufficient cooling of the parts where the molten metal is eroded violently in the inner runner caused by the casting conditions.
Nine erosions
There are pits or ridges in some parts of the die-casting parts.
The reasons are as follows:
- Improper setting of the gate sprue position;
- The cooling conditions are not good.
ten cracks
When the casting is placed in an alkaline solution, the cracks will appear dark gray. The damage and cracking of the metal matrix are linear or wavy, with narrow and long lines, and tend to develop under the action of external forces.
The reasons are as follows:
- The iron content in the alloy is too high or the silicon content is too low; the content of harmful impurities in the alloy is too high, which reduces the plasticity of the alloy; aluminum-silicon alloys and aluminum-silicon-copper alloys contain too much zinc or copper; aluminum-magnesium alloys contain Too much magnesium;
- The mold retention time is too short and the pressure holding time is short; the wall thickness of the casting changes drastically;
- The local tightening force is too large and the force is uneven during ejection.
Aluminum alloy die-casting processing process:
- Melting and refining
- Die casting and forming
- shaping and trimming
- machining
- Cleaning and cleaning
- Assembly
In the production process of die-casting parts, cleaning or surface pretreatment is required, including die-casting demoulding, machining, and cleaning. It is worth noting that the processing difficulty of workpieces of different complexity is different, and the requirements for cleaning are also different. To control the damage to the workpiece to a minimum, the property requirements of the cleaning products are more stringent.
Die casting link
Problems: mold sticking, scale accumulation, bubbling, cracking, etc.
During the die-casting process, because the mold is constantly heated by high-temperature liquid metal, it is easy to adhere to the die-casting parts, and even defects such as bubbling, cracking, and thermal cracking may occur. In order to solve the above problems, release agents are often used in workpiece production to reduce damage.
Release agent is a functional substance between the mold and the finished product. It can form a uniform release film on the surface of the mold, allowing the die-casting parts to be smoothly removed from the mold, ensuring the integrity and post-processability of the product. . Therefore, choosing an appropriate release agent formula can minimize the adhesion between the casting and the mold.